XPS Reference Pages

This site contains information gained from decades of X-ray photoelectron spectroscopy (XPS) analyses of an enormous variety of samples analyzed at Surface Science Western laboratories located at the Western University (London, Ontario). Originally this site was designed as a place for students and our clients to access valuable tips and information. It has since been opened to all those interested in the XPS technique. Summaries of literature data, relevant references and unpublished data taken of well characterized standard samples are presented. Also curve-fitting tips, instrument set-up tips (specifically for the Kratos AXIS Supra, Ultra and Nova), and CasaXPS tips pertaining to questions we normally get from our students and clients, and other odd bits of information are presented.




The fine print:
Surface Science Western and the University of Western Ontario does not warranty any of the information shown at this site. Any use of this data in scientific publications or other forms should include referencing to the originally published data referenced herein.

Magnesium 2p and Auger Parameter Values

Magnesium 2p binding energy and modified Auger parameter values are shown in Table 1. It is worth noting that accounting for the difference between charge referencing procedures is vital for correct analysis of magnesium compounds (especially for MgO and Mg(OH)2) [1]. For MgO, the peak position for the Mg 2p transition is 49.4 eV when charge referenced to adventitious carbon at 284.8 eV, and 50.8 when referenced to the Mg 2p metal peak at 49.73 eV (or grounded). This has led to a lot of confusion regarding the Mg 2p peak positions to use for analysis. The results from a consistently analyzed dataset are shown in Table 1 together with compiled literature values [1]. Since the chemical sensitivity of the Mg 2p transition is low for magnesium the Auger parameter and anion signals are particularly important to consider for improved speciation.

Table 1: Experimental and literature values for the Mg 2p binding energy and the modified Auger parameter for different magnesium compounds. Subscripts and superscripts: “sc” denotes single crystal; “g” denotes grounded and no charge correction was performed; “Mg” denotes floated and the Mg 2p metal peak was used as a charge reference at 49.73 eV; “O 1s” denotes floated and the O 1s lattice peak of MgO or Mg(OH)2 was used as a charge reference at 531.1 eV and 532.7 eV, respectively. Samples with no superscript were floated, and adventitious carbon was used as a charge reference at 284.8 eV. 

The anion fitting parameters—binding energy, peak width, and line shape—obtained from fitting reference samples are reported in Table 2 from a consistently analyzed data set [1]. The O 1s signal can be used to separate MgO and Mg(OH)2 despite their overlapping Mg 2p signals. The O 1s peak position of Mg(OH)2 is +1.6 eV with respect to the main lattice peak of MgO. However, the peak position for Mg(OH)2 can overlap with other environments such as the MgO defective oxide and adventitious carbon, which may need to be accounted for in the analysis.

Table 2: Overview of anion fitting parameters, binding energy, peak width, and line shape, from reference data. Subscripts and superscripts: “sc” denotes single crystal;  “g” denotes grounded and no charge correction was performed; “Mg” denotes floated and the Mg 2p metal peak was used as a charge reference at 49.73 eV; “ref” denotes reference values when charge referencing to the O 1s lattice peak. Samples with no superscript were floated, and adventitious carbon was used as a charge reference at 284.8 eV. 

Reference:

Magnesium Induced Ghost Peaks

Ghost peaks occur when internal X-rays are produced within the sample, ejecting a detectable number of core-level photoelectrons. Since these internally produced X-rays have lower energy than the source X-rays, they eject photoelectrons with a lower kinetic energy (higher apparent binding energy). While ghost peaks in many cases appear with low intensity and therefore do not generally interfere with XPS analysis, they may cause confusion during peak assignment.

Ghost peaks are often observed for magnesium-rich samples from the Mg Kα emission lines (X-rays produced when a valence electron fills the Mg 1s core hole). The average photon energy of these lines is 1253.6 eV, and the position of the ghost peaks on the binding energy scale is dependent on the X-ray source. For example, the Mg Kα induced O 1s ghost peak is seen in the XPS spectra of Mg(OH)2 at 765.7 eV, when using an Al Kα source (1486.7 eV). This peak position is shifted by 233.1 eV, which is the energy difference between internal and source X-rays (Figure 1). 

Alternatively, this can also be calculated as follows: the Mg K X-ray induced peak for O 1s is found at a binding energy of ~ 765.7 eV, as the kinetic energy of these photoelectrons would be 1253.6 eV (Mg Kα X-rays) - 532.6 eV (O 1s B.E.) = 721.0 eV. Thus, they would then be seen as a peak at a binding energy of 1486.7 ( Al K(α) X-rays) - 721.0 eV = 765.7 eV. Similarly, the C 1s Mg X-ray induced peak would be at a binding energy of ~517 eV.

Also of note for spectra of magnesium-rich samples: Mg Auger structure can be found at ~242 eV, which is not a ghost peak and often not noted in most libraries (Figure 1, Mg KLL-2) and may cause confusion during survey scan peak assignment.  

Figure 1. Survey spectrum of Mg(OH)2 powder where the O 1s ghost peak is clearly visible at 765.7 eV. The figure is reproduced from reference [1]. 

XPS Detection Limits

In general, detection limits for XPS range from 0.1 to 1 atomic percent.  However there are cases where limits could be much better or much worse.  An article from Alexander Shard [1] gives an excellent look at detection limits in over 6000 binary systems for both Al and Mg X-ray sources.  In such systems a heavy element, such as gold, in a light element matrix, say carbon, would have detection limits closer to 0.01 atomic percent.  For the opposite situation, carbon in a gold matrix, detection limits for carbon would be around 3 atomic percent.  Spectral overlaps can also degrade detection limits significantly and are incorporated into the tables presented.  Overlaps with Auger peaks can be overcome by changing X-ray sources used (i.e. using Mg K instead of Al K).  One can also work with advanced curve-fitting techniques to overcome some of these overlap issues.

Download printable PDF of detection limits for Mg X-ray spectra.

XPS detection limits using Al K(alpha) radiation [1].
Reference:
[1] A.G. Shard, Surf. Interface Anal. 46 (2014) 175-185.

Carbon 1s for Organic Compounds

The seminal work of Graham Beamson and Dave Briggs in their "High Resolution XPS of Organic Polymers – The Scienta ESCA300 Database" has been utilized since 1992 as an invaluable resource for the XPS analysis of polymers and organic materials.  A summary of carbon 1s binding energies for organic functional groups from this work are presented here. The original work calibrates the binding energy scale to 285.0 eV for aliphatic carbon C 1s. The values presented here are now calibrated to 284.8 eV for aliphatic carbon, in line with recent results [2].  

Figure 1. Summary of the mean, maximum, and minimum carbon 1s binding energies for different organic functionalities according to the work of Beamson and Briggs [1].  Binding energy calibration presented here have been adjusted to the main aliphatic C 1s peak at 284.8 eV.

Table 1. Summary of the mean, maximum, and minimum carbon 1s binding energies for different organic functionalities according to the work of Beamson and Briggs [1].  Binding energy calibration presented here have been adjusted to the main aliphatic C 1s peak at 284.8 eV.


Table 2. Summary of beta shift effects from Beamson and Briggs (Appendix 2) [1].

The effects of various functional groups on beta carbon binding energies can be significant (Table 2).  Note that, in this context, the alpha carbon is the carbon directly attached to the functional group, and the beta carbon is attached to the alpha carbon. These effects have been included in the refinement of the binding energy value for the aliphatic carbon component in adventitious carbon [2]. 

References:
[1] G. Beamson, D. Briggs, High Resolution XPS of Organic Polymers - The Scienta ESCA300 Database, Wiley Interscience, 1992, Appendices 1 and 2.
[2] L.H. Grey, H.-Y. Nie, M.C. Biesinger, Appl. Surf. Sci. 653 (2024) 159319.

Oxygen 1s for Organic Compounds

Figure 1. Summary of the mean, maximum, and minimum oxygen 1s binding energies for different organic functionalities according to the work of Beamson and Briggs [1].  Binding energy calibration presented here have been adjusted to the main aliphatic C 1s peak at 284.8 eV [2].

Figure 2. Oxygen 1s binding energy means and ranges for various organic compound types. Plotted from data supplied in Beamson and Briggs [1]. Referenced to main aliphatic C 1s peak at 285.0 eV as in the original source data.

Additional Notes: 
C-OH (aliphatic) Ref to C 1s at 284.8 eV: Average 532.7 eV, Min. 532.5 eV, Max. 532.9 eV
C-OH (aliphatic) Ref to C 1s at 285.0 eV: Average 532.9 eV, Min. 532.7 eV, Max. 533.1 eV
C-OH (aromatic) Ref to C 1s at 284.8 eV: 533.4 eV 
C-OH (aromatic) Ref to C 1s at 285.0 eV: 533.6 eV 

Also note that Si 2p3/2 for PDMS (silicone) is at 101.79 eV (Si 2p = 102.0 eV) with the C 1s at 284.38 eV and O 1s at 532.00 eV (referenced to aliphatic C at 285.0 eV).  If we shift the C 1s to 285.0 eV then Si 2p3/2 is at 102.41 eV (Si 2p = 102.6 eV) and O 1s is at 532.62 eV for silicone. If we then shift the C 1s to 284.8 eV then Si 2p3/2 is at 102.21 eV (Si 2p = 102.4 eV) and O 1s is at 532.42 eV for silicone.

References:
[1] G. Beamson, D. Briggs, High Resolution XPS of Organic Polymers - The Scienta ESCA300 Database, Wiley Interscience, 1992, Appendices 3.1 and 3.2.

Calculating Oxygen Content from Adventitious Carbon 1s Spectra

Adventitious carbon (AdC) is commonly detected in X-ray photoelectron spectroscopy (XPS) analyses of most samples. While AdC can be beneficial in some cases, such as for charge correction purposes during the analysis of insulators, its associated C–O functionalities can complicate the interpretation of O 1s spectra. Accurately accounting for AdC’s contribution within the O 1s spectrum is essential but challenging due to significant spectral overlap and poorly resolved components in the high-resolution O 1s spectrum.

Rather than assigning multiple components without clear physical meaning—potentially leading to misinterpretations—incorporating stoichiometry offers a more reliable approach to improving data accuracy. However, applying stoichiometry can be tedious and challenging, particularly for novice users.

A recently published article [1] describes an approximation to enhance oxygen spectra interpretation by estimating oxygen linked to AdC. This publication provides background information, key assumptions, and an easy-to-use Excel calculator to assist XPS researchers in analyzing their own O 1s spectra.

This approach is particularly useful for accurately quantifying survey spectra when AdC influence must be minimized and for modelling high-binding-energy components in the oxygen 1s spectrum. The latter example is important to many transition metal oxides which have overlapping hydroxide and/or defect oxide components in the same binding energy window. Detailed examples of these applications are presented and discussed in reference [1]. These types of calculations were originally introduced in [2].

This Excel based calculator (also available at supplementary material in [1]) takes information from the survey and high resolution carbon 1s spectra and determines the amount of oxygen that is present from adventitious carbon species. This amount can then be deducted from the overall oxygen concentration.
(Note: you must download the file to Excel to use it - it is locked in Google Docs).

Caesium

 

Cs 3d5/2 binding energy values.

Note: Cs 3d5/2 - 3d3/2 splitting is 13.94 eV

Cs 3s: 1219 eV

Cs 3p3/2: 1002 eV

Cs 3p1/2: 1069 eV

Cs 4s: 234 eV

Cs 4p3/2: 161 eV

Cs 4p1/2: 173 eV

Cs 4d5/2: 77 eV

Cs 4d3/2: 80 eV

Cs 5s: 25 eV

Cs M5N45N45: 931 eV (Al)

Cs M4N45N45: 918 eV (Al)

Advanced Analysis of Indium

Analysing indium and indium-based compounds using X-ray Photoelectron Spectroscopy is challenging due to only slight shifts in the binding energies of the commonly used In 3d5/2 core line. A recent paper shares a comprehensive set of reference data for indium and its compounds, covering the In 3d, 3p, and 4d core lines, the In MNN Auger signal, as well as relevant counter ion signals [1]. Valuable tools, such as the modified Auger parameter and chemical state (Wagner) plots, which aid in differentiating indium species are also discussed.

Figure 1 and Table 1 present average literature values for the In 3d5/2 core line, highlighting both the average and standard deviations. These values illustrate the apparent challenge in distinguishing between various indium compounds. Factors like natural line widths, line shapes, and potential errors in charge correction add further complexity to accurate speciation.

Figure 1. Average In 3d5/2 literature values for indium compounds. 

Table 1. Average In 3d5/2 literature values for indium compounds.

Experimental data (Figure 2 and Table 2) presents a similar trend, underscoring that the In 3d5/2 core line alone is not enough to reliably distinguish between indium species. Notably, the In 3d5/2 core line of indium oxides shows variable asymmetry in line shape, which has led to differing interpretations in the literature. Some researchers attribute the high binding energy component to hydroxide or oxy-hydroxide species, while others suggest that it reflects electronic properties (screening effects). The current experiments [1] support the view that screening effects play an important role in this asymmetry. Excellent studies on these screening effects have been conducted by Körber [2] and Harvey [3].

Figure 2 In 3d spectra from [1].

Table 2. Experimental In 3d5/2 values from [1].

The In M4,5N4,5N4,5 transitions show a broader range of binding energy than the In 3d5/2 core level, making it better suited for accurate speciation, particularly by making use of the modified Auger parameter (Figure 3 and Table 3). In mixed-system analysis, i.e., a system containing multiple indium species, both the position and shape of the In M4,5N4,5N4,5 Auger electron signal can useful for speciation. Béchu and Fairley have provided an excellent discussion on the application of nonlinear and linear least-squares fitting methods to the In M4,5N4,5N4,5 signal, specifically for the oxidation of InSb [4]. Table 4 presents the fitting parameters needed to reproduce the M4,5N4,5N4,5 line shapes in order to fit complex experimental envelopes.

Figure 3. In MNN spectra for various indium compounds [1]. For reference, vertical lines indicating the kinetic energy (MNN) for metallic indium have been overlaid in each tile. Note that the additional signal present for InPO4 at 414.7 eV was due to Na contamination.

Table 3. In M4N4,5N4,5 and modified Auger parameter values [1]. 

Table 4. In MNN Auger peak fitting parameters [1].

Considering the information presented above, a comprehensive interpretation of XPS data involving indium and its compounds should involve a combination of the available data, including survey spectra (i.e., stoichiometry), the In 3d5/2 and In M4N4,5N4,5 Auger spectra, as well as the relevant counterion spectra (see [1]). For systems containing multiple indium compounds, the position and shape of the M4,5N4,5N4,5 transition can offer a more accurate approach than using the 3d5/2 core line alone.

References:
[1] J.D. Henderson, L.P. Pearson, H-Y. Nie, M.C. Biesinger, Surf. Interface Anal. 57 (2024) 81. https://doi.org/10.1002/sia.7356 
[2] C. Körber (et al.), Phys. Rev. B, 81 (2010) 165207
[3] S.P. Harvey (et al.), J. Phys. D Appl. Phys., 39 (2006) 3959.
[4] S. Béchu and N. Fairley, J. Vac. Sci. Technol. A, 42 (2024) 013202.

Iron

For the analysis of photoelectron spectra of relatively pure iron oxides, one can use peak shape and peak binding energy comparisons to standard compounds to derive oxide composition. McIntyre and Zetaruk’s [1] paper is widely cited and is still an excellent starting point for qualitative iron oxide determination. Pratt et al. [2] used a series of multiplet peaks to curve fit oxidized iron sulfide (pyrrhotite) surfaces.

Grosvenor et al.[3] fitted the various iron oxide, hydroxide and halide peak shapes with a close approximation of the Gupta and Sen[4] multiplet structure. Multiplet FWHM, splittings and weightings are presented. An analysis of satellite to main peak separation is also given. All Fe(II) (high spin only as low spin Fe(II) does not exhibit multiplet splitting) and Fe(III) species can be fitted with Gupta and Sen multiplet structure. Variation in peak spacing and intensity occur for different ligands. Broad satellite peaks of varying intensities at binding energies above the main Fe 2p3/2 structure are present in the spectra for all high spin compounds. However paper [3] only presents the main multiplet lines, excluding the details needed to fit the broader higher binding energy satellite structures.

Table 1 [5] presents full fitting parameters including the multiplet and satellite structure. FWHM values are reported for 10 eV pass energy only. To accommodate lower resolution settings slightly broader peaks would be necessary for best fit values. For these fits a Shirley background encompassing only the 2p3/2 portion of the spectrum is used. Also included in this Table are new spectral fitting parameters for FeCr2O4 and NiFe2O4, species that are important for the examination of oxide films on Fe-Cr-Ni alloys, as well as data for new analyses of α-Fe2O3 and γ-Fe2O3[5]. Fitting parameters for FeCO3, which has been noted in certain corrosion products, are also presented in Table 1. These analyses were collected from a mineral sample of siderite (cleaved in vacuum). Carbon 1s binding energy for FeCO3 is at 290.1 eV. The many spectra are best viewed in the original papers - see links in reference section.

New! Modified/updated fitting parameters for FeO, FeOOH and Fe3O4 are now included in Table 1 from work presented in reference [6]. In particular the analysis and fitting of FeO is improved substantially as the new FeO standard, sputter cleaned with a GCIS (not available during the original work in [3,5]), is free of low levels of surface Fe2O3/Fe3O4 contamination.


Table 1. Fe 2p3/2 spectral fitting parameters: binding energy (eV), percentage of total area, FWHM value (eV) and spectral component separation (eV) [5,6].

While these values [5] and reference spectra [1,3,5] will be useful for identification of pure oxide or oxy-hydroxide species, curve fitting of mixed systems quickly becomes complicated due to spectral overlaps. For example, it can be seen that various Fe(III) compounds have a similar range of Fe 2p binding energies and vary mostly in peak shape and satellite intensities. Any attempt at fitting two or more Fe(III) species to a spectrum will consequently contain an inherent degree of error. As well, overlap of the Fe(III) satellite structure with the Fe(0) and Fe(II) Fe 2p1/2 portion of the spectrum will result in setting the higher binding energy background endpoint placement at a point that will not cover the satellite structure of the Fe(III) species. This will require any fitting of mixed chemical state systems containing Fe(III) species to omit the higher binding energy Fe(III) satellite (e.g. Fe2O3, FeOOH) from the envelope of peaks. This will again increase the error associated with the curve fitting.  Finally, determination of the Fe species present, especially in a mix of Fe(III) species, should include corroborating evidence from O 1s analysis and even other analytical techniques such as Raman spectroscopy or, for thin crystalline films, grazing angle XRD. Some examples of fittings in mixed species samples are presented in [5].

Compared to the other transition metal species, the complex multiple species fitting of Fe is the most problematic. With so many possible species having overlapping binding energies erroneous interpretation can result. A sample with two distinct species can likely be fitted accurately, three species much less so, while four or more species must be looked at as indicative but unreliable. 

New! Recent work [6,7] has demonstrated the utility of these methodologies, with extremely good chemical state speciation achieved for oxide/hydroxide mixtures.  For metal/oxide/hydroxide mixtures, good success was found for low levels of metal content.  As the amount of metal grows (particularly above 25%) the amount of Fe(II) species tends to be underestimated. Results from the original curve-fittings from [5] were improved, particularly for FeO.  This work again emphasizes that the better the pure compound spectrum is, the better the final curve-fitting results!

Further work from Hughes et al. [8], published in the journal Corrosion Science in 2025, highlights the widespread erroneous analysis of the Fe 2p peak in XPS studies in corrosion science. It shows again the need for best practices when it come to fitting Fe 2p XPS spectra.

References:
[1] N.S. McIntyre, D.G. Zetaruk, Anal. Chem. 49 (1977) 1521.
[2] A.R. Pratt, I.J. Muir, H.W. Nesbitt, Geochim. Cosmochim. Acta 58 (1994) 827.
[3] A.P. Grosvenor, B.A. Kobe, M.C. Biesinger, N.S. McIntyre, Surf. Interface Anal. 36 (2004) 1564.
[4] R.P. Gupta, S.K. Sen, Phys Rev. B 12 (1975) 15.
[5] M.C. Biesinger, B.P. Payne, A.P. Grosvenor, L.W.M. Lau, A.R. Gerson, R.St.C. Smart, Appl. Surf. Sci. 257 (2011) 2717.
[6] A.E. Hughes, C.D. Easton, T.R. Gengenbach, M.C. Biesinger, M. Laleh, (2024) JVST A, 42 (2024) 053205.
[7] A.E. Hughes, C.D. Easton, T.R. Gengenbach, M.C. Biesinger, M. Laleh, (2024) JVST A, 42 (2024) 053206.
[8] A.E. Hughes, C.D. Easton, P.R. Anusuyadevi, T.J. Raeber, N.C. Wilson, A. Mol, Corr. Sci. 257 (2025) 113357.