Pages

▼

Iron

For the analysis of photoelectron spectra of relatively pure iron oxides, one can use peak shape and peak binding energy comparisons to standard compounds to derive oxide composition. McIntyre and Zetaruk’s [1] paper is widely cited and is still an excellent starting point for qualitative iron oxide determination. Pratt et al. [2] used a series of multiplet peaks to curve fit oxidized iron sulfide (pyrrhotite) surfaces.

Grosvenor et al.[3] fitted the various iron oxide, hydroxide and halide peak shapes with a close approximation of the Gupta and Sen[4] multiplet structure. Multiplet FWHM, splittings and weightings are presented. An analysis of satellite to main peak separation is also given. All Fe(II) (high spin only as low spin Fe(II) does not exhibit multiplet splitting) and Fe(III) species can be fitted with Gupta and Sen multiplet structure. Variation in peak spacing and intensity occur for different ligands. Broad satellite peaks of varying intensities at binding energies above the main Fe 2p3/2 structure are present in the spectra for all high spin compounds. However paper [3] only presents the main multiplet lines, excluding the details needed to fit the broader higher binding energy satellite structures.

Table 1 [5] presents full fitting parameters including the multiplet and satellite structure. FWHM values are reported for 10 eV pass energy only. To accommodate lower resolution settings slightly broader peaks would be necessary for best fit values. For these fits a Shirley background encompassing only the 2p3/2 portion of the spectrum is used. Also included in this Table are new spectral fitting parameters for FeCr2O4 and NiFe2O4, species that are important for the examination of oxide films on Fe-Cr-Ni alloys, as well as data for new analyses of α-Fe2O3 and γ-Fe2O3[5]. Fitting parameters for FeCO3, which has been noted in certain corrosion products, are also presented in Table 1. These analyses were collected from a mineral sample of siderite (cleaved in vacuum). Carbon 1s binding energy for FeCO3 is at 290.1 eV. The many spectra are best viewed in the original papers - see links in reference section.

New! Modified/updated fitting parameters for FeO, FeOOH and Fe3O4 are now included in Table 1 from work presented in reference [6]. In particular the analysis and fitting of FeO is improved substantially as the new FeO standard, sputter cleaned with a GCIS (not available during the original work in [3,5]), is free of low levels of surface Fe2O3/Fe3O4 contamination.


Table 1. Fe 2p3/2 spectral fitting parameters: binding energy (eV), percentage of total area, FWHM value (eV) and spectral component separation (eV) [5,6].

While these values [5] and reference spectra [1,3,5] will be useful for identification of pure oxide or oxy-hydroxide species, curve fitting of mixed systems quickly becomes complicated due to spectral overlaps. For example, it can be seen that various Fe(III) compounds have a similar range of Fe 2p binding energies and vary mostly in peak shape and satellite intensities. Any attempt at fitting two or more Fe(III) species to a spectrum will consequently contain an inherent degree of error. As well, overlap of the Fe(III) satellite structure with the Fe(0) and Fe(II) Fe 2p1/2 portion of the spectrum will result in setting the higher binding energy background endpoint placement at a point that will not cover the satellite structure of the Fe(III) species. This will require any fitting of mixed chemical state systems containing Fe(III) species to omit the higher binding energy Fe(III) satellite (e.g. Fe2O3, FeOOH) from the envelope of peaks. This will again increase the error associated with the curve fitting.  Finally, determination of the Fe species present, especially in a mix of Fe(III) species, should include corroborating evidence from O 1s analysis and even other analytical techniques such as Raman spectroscopy or, for thin crystalline films, grazing angle XRD. Some examples of fittings in mixed species samples are presented in [5].

Compared to the other transition metal species, the complex multiple species fitting of Fe is the most problematic. With so many possible species having overlapping binding energies erroneous interpretation can result. A sample with two distinct species can likely be fitted accurately, three species much less so, while four or more species must be looked at as indicative but unreliable. 

New! Recent work [6,7] has demonstrated the utility of these methodologies, with extremely good chemical state speciation achieved for oxide/hydroxide mixtures.  For metal/oxide/hydroxide mixtures, good success was found for low levels of metal content.  As the amount of metal grows (particularly above 25%) the amount of Fe(II) species tends to be underestimated. Results from the original curve-fittings from [5] were improved, particularly for FeO.  This work again emphasizes that the better the pure compound spectrum is, the better the final curve-fitting results!

Further work from Hughes et al. [8], published in the journal Corrosion Science in 2025, highlights the widespread erroneous analysis of the Fe 2p peak in XPS studies in corrosion science. It shows again the need for best practices when it come to fitting Fe 2p XPS spectra.

References:
[1] N.S. McIntyre, D.G. Zetaruk, Anal. Chem. 49 (1977) 1521.
[2] A.R. Pratt, I.J. Muir, H.W. Nesbitt, Geochim. Cosmochim. Acta 58 (1994) 827.
[3] A.P. Grosvenor, B.A. Kobe, M.C. Biesinger, N.S. McIntyre, Surf. Interface Anal. 36 (2004) 1564.
[4] R.P. Gupta, S.K. Sen, Phys Rev. B 12 (1975) 15.
[5] M.C. Biesinger, B.P. Payne, A.P. Grosvenor, L.W.M. Lau, A.R. Gerson, R.St.C. Smart, Appl. Surf. Sci. 257 (2011) 2717.
[6] A.E. Hughes, C.D. Easton, T.R. Gengenbach, M.C. Biesinger, M. Laleh, (2024) JVST A, 42 (2024) 053205.
[7] A.E. Hughes, C.D. Easton, T.R. Gengenbach, M.C. Biesinger, M. Laleh, (2024) JVST A, 42 (2024) 053206.
[8] A.E. Hughes, C.D. Easton, P.R. Anusuyadevi, T.J. Raeber, N.C. Wilson, A. Mol, Corr. Sci. 257 (2025) 113357.