To calculate a new R.S.F. for other elements/core lines (for the R.S.F. table type used by the CasaXPS/ Kratos Supra/Ultra/Nova combination) the following formula are used.
RSFp3/2 = RSFp * 2/3
RSFp1/2 = RSFp * 1/3
RSFd5/2 = RSFd * 3/5
RSFd3/2 = RSFd * 2/5
RSFf7/2 = RSFf * 4/7
RSFf5/2 = RSFf * 3/7


Table 1. Relative sensitivity factors for CasaXPS / Kratos Supra / Ultra / Nova.a) Use a window of 298-300eV (see Mg link for more details)
b) Calculated from BaTiO3 standard sample
c) New value from standard sample
d) Calculated values based on RSF's from SSX-100 XPS (U 4f = 48.86, Th 4f= 42.75) ratiod to Th 4f from Kratos instruments (Th 4f = 12.75). 48.86/42.75 = RSF(U 4f Kratos)/12.75; RSF(U 4f Kratos) = 14.544. It would be useful if this value could be confirmed with a well characterized UO2 sample.